CAMPUS® datasheet | Ultramid® A3Z HP


This datasheet of Ultramid® A3Z HP from BASF is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Ultramid® A3Z HP | PA66 | BASF
Product Texts
Impact-modified and stabilized injection moulding grade for components and housing with good low temperature impact resistance.
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 1900 / - MPa ISO 527-1/-2
Yield stress 50 / - MPa ISO 527-1/-2
Yield strain 5 / - % ISO 527-1/-2
Nominal strain at break 45 / - % ISO 527-1/-2
Charpy impact strength (+23°C) N / - kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) N / - kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 90 / - kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 28 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 262 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 64 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 170 / * °C ISO 75-1/-2
Other propertiesdry / condUnitTest Standard
Density 1070 / - kg/m³ ISO 1183
Characteristics
Processing
Injection Molding
Regional Availability
North America
Other text information
Injection molding
Max. Water content: 0.20%
Product is supplied in sealed containers and
drying prior to molding is not required. If drying
becomes necessary, a dehumidifying or desiccant dryer
operating at 80 degC (176 degF) is recommended. Drying time is
dependent on moisture level, but 2-4 hours is generally
sufficient.
Further information concerning safe handling procedures
can be obtained from the Material Safety Data Sheet.
Alternatively, please contact you r BASF representative.
PROCESSING
Melt Temperature 280-304 degC (536-580 degF)
Mold Temperature 60-100 degC (140-212 degF)
Injection and Packing Pressure 35-125 bar (500-1500 psi)
Back Pressure 0-0.35 MPa (0-50 psi)
Screw Speed 40-80 rpm
Screw Compression Ratio 3:1 to 4:1

This product can be processed over a wide range of mold
temperatures; however, for applications where aesthetics are
critical, a mold surface temperature of 60-100 degC (140-212 degF)
is recommended.

Injection pressure controls the filling of the part and should
be applied for 90% of ram travel. Packing pressure affects
the final part and can be used effectively in controlling
sink marks and shrinkage. It should be applied and maintained
until the gate area is completely frozen off.
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact your local BASF
representative or

BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)