This datasheet of Ultramid® B3WGM24 BK30564 from BASF is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Ultramid® B3WGM24 BK30564 | PA6-(GF+MD)30 | BASF
Product Texts
Glass-fibre and mineral reinforced heat stabilized injection moulding grade for industrial articles having medium to high rigidity and high dimensional stability, used e.g. for automobile engine covers, housings and automotive door handles.
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 9300 / 4200 MPa ISO 527-1/-2
Stress at break 120 / 55 MPa ISO 527-1/-2
Strain at break 3 / 10 % ISO 527-1/-2
Charpy impact strength (+23°C) 52 / 60 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 50 / 45 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 7 / 13 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 5 / 5 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 220 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 195 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 215 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion (parallel) 38 / * E-6/K ISO 11359-1/-2
Electrical propertiesdry / condUnitTest Standard
Relative permittivity (1MHz) 3.9 / 6.2 - IEC 60250
Dissipation factor (1MHz) 200 / 2000 E-4 IEC 60250
Volume resistivity 1E13 / 1E10 Ohm*m IEC 60093
Surface resistivity * / 1E10 Ohm IEC 60093
Comparative tracking index - / 400 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 7.2 / * % Sim. to ISO 62
Humidity absorption 2.3 / * % Sim. to ISO 62
Density 1370 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
Viscosity number 140 / * cm³/g ISO 307, 1157, 1628
Diagrams
Stress-strain , Ultramid® B3WGM24 BK30564, PA6-(GF+MD)30, BASF
Secant modulus-strain , Ultramid® B3WGM24 BK30564, PA6-(GF+MD)30, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants, Release agent
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
North America
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 10 h

PROCESSING
injection molding, Melt temperature, range: 270 - 290 °C
injection molding, Mold temperature, range: 80 - 90 °C

Max. Water content: 0.10%
Product is supplied in sealed containers and
drying prior to molding is not required. If drying
becomes necessary, a dehumidifying or desiccant dryer
operating at 80 degC (176 deg F) is recommended. Drying time is
dependent on moisture level, but 2-4 hours is generally
sufficient.
Further information concerning safe handling procedures
can be obtained from the Material Safety Data Sheet.
Alternatively, please contact your BASF representative.
PROCESSING
Melt Temperature 270-295 degC (518-563

degF)
Mold Temperature 80-95 degC (176-203 degF)
Injection and Packing Pressure 35-125 bar (500-1500 psi)

This produc t can be processed over a wide range of mold
temperatures; however, for applications where aesthetics are
critical, a mold surface temperature of 80-95 degC (176-203 degF)
is recommended.

Injection pressure controls the filling of the part and should
be applied for 90% of ram travel. Packing pressure affects
the final part and can be used effectively in controlling
sink marks and shrinkage. It should be applied and maintained
until the gate area is co mpletely frozen off.

Back pressure can be utilized to provide uniform melt consistency
and reduce trapped air and gas. Minimal back pressure should be

utilized to
prevent glass breakage.

Fast fill rates are recommended to insure uniform melt
delivery to the cavity and prevent premature freezing. Surface
appearance is directly affected by injection rate.
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact your local BASF
representative or

BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991