View list of
Interactive Graphics for LTHA Diagrams?
FREE DOWNLOAD
Interested inInteractive Graphics for LTHA Diagrams?
The CAMPUS desktop version
offers extended functionality!CAMPUS® datasheet | Ultrason® E 3010 NAT
This datasheet of Ultrason® E 3010 NAT from BASF is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
You may contact the supplier for more information about this grade.
Ultrason® E 3010 NAT | PESU | BASF
Product Texts
Unreinforced, higher viscosity injection moulding and extrusion grade, tougher and with improved chemical resistance.
Abbreviated designation according to ISO 1043-1: PESU
Abbreviated designation according to ISO 1043-1: PESU
| Rheological properties | dry / cond | Unit | Test Standard |
| Melt volume-flow rate (MVR) | 35 / * | cm³/10min | ISO 1133 |
| Temperature | 360 / * | °C | ISO 1133 |
| Load | 10 / * | kg | ISO 1133 |
| Molding shrinkage (parallel) | 0.8 / * | % | ISO 294-4, 2577 |
| Molding shrinkage (normal) | 0.9 / * | % | ISO 294-4, 2577 |
| Mechanical properties | dry / cond | Unit | Test Standard |
| Tensile Modulus | - / 2700 | MPa | ISO 527-1/-2 |
| Yield stress | - / 90 | MPa | ISO 527-1/-2 |
| Yield strain | - / 6.7 | % | ISO 527-1/-2 |
| Tensile creep modulus (1h) | * / 2800 | MPa | ISO 899-1 |
| Tensile creep modulus (1000h) | * / 2700 | MPa | ISO 899-1 |
| Charpy impact strength (+23°C) | - / N | kJ/m² | ISO 179/1eU |
| Charpy impact strength (-30°C) | - / N | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | - / 7.5 | kJ/m² | ISO 179/1eA |
| Charpy notched impact strength (-30°C) | * / 7.5 | kJ/m² | ISO 179/1eA |
| Thermal properties | dry / cond | Unit | Test Standard |
| Glass transition temperature (10°C/min) | 228 / * | °C | ISO 11357-1/-2 |
| Temp. of deflection under load (1.80 MPa) | 207 / * | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 218 / * | °C | ISO 75-1/-2 |
| Vicat softening temperature (50°C/h 50N) | 215 / * | °C | ISO 306 |
| Coeff. of linear therm. expansion (parallel) | 52 / * | E-6/K | ISO 11359-1/-2 |
| Burning Behav. at 1.5 mm nom. thickn. | V-0 / * | class | IEC 60695-11-10 |
| Thickness tested | 1.5 / * | mm | IEC 60695-11-10 |
| UL recognition | UL / * | - | - |
| Burning Behav. 5V at thickness h | 5VA / * | class | IEC 60695-11-20 |
| Thickness tested | 3.0 / * | mm | IEC 60695-11-20 |
| UL recognition | UL / * | - | - |
| Oxygen index | 42.5 / * | % | ISO 4589-1/-2 |
| Electrical properties | dry / cond | Unit | Test Standard |
| Relative permittivity (100Hz) | * / 3.9 | - | IEC 60250 |
| Relative permittivity (1MHz) | * / 3.8 | - | IEC 60250 |
| Dissipation factor (100Hz) | * / 17 | E-4 | IEC 60250 |
| Dissipation factor (1MHz) | * / 140 | E-4 | IEC 60250 |
| Volume resistivity | * / >1E13 | Ohm*m | IEC 60093 |
| Surface resistivity | * / >1E15 | Ohm | IEC 60093 |
| Electric strength | * / 34 | kV/mm | IEC 60243-1 |
| Comparative tracking index | * / 125 | - | IEC 60112 |
| Other properties | dry / cond | Unit | Test Standard |
| Water absorption | 2.2 / * | % | Sim. to ISO 62 |
| Humidity absorption | 0.8 / * | % | Sim. to ISO 62 |
| Density | 1370 / - | kg/m³ | ISO 1183 |
| Material specific properties | dry / cond | Unit | Test Standard |
| Viscosity number | 66 / * | cm³/g | ISO 307, 1157, 1628 |
| Rheological calculation properties | Value | Unit | Test Standard |
| Density of melt | 1230 | kg/m³ | - |
| Thermal conductivity of melt | 0.18 | W/(m K) | - |
| Spec. heat capacity melt | 1950 | J/(kg K) | - |
| Ejection temperature | 200 | °C | - |
| Test specimen production | Value | Unit | Test Standard |
| Injection Molding, melt temperature | 370 | °C | ISO 294 |
| Injection Molding, mold temperature | 160 | °C | ISO 10724 |
| Injection Molding, injection velocity | 200 | mm/s | ISO 294 |
| Injection Molding, pressure at hold | 70 | MPa | ISO 294 |
Diagrams
Characteristics
Processing
Injection Molding, Film Extrusion, Profile Extrusion, Sheet Extrusion, Blow Molding, Thermoforming
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .02 %
Pre/Post-processing, Pre-drying, Temperature: 140 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
injection molding, Melt temperature, range: 350 - 390 °C
injection molding, Melt temperature, recommended: 370 °C
injection molding, Mold temperature, range: 140 - 180 °C
injection molding, Mold temperature, recommended: 160 °C
Pretreatment
Drying temperature: 130 - 150°C
Drying time: minimum 4h
recommended dryer: vaccum or dry air dryer
maximum moisture: 0,02 - 0,05%
Ultrason® can be injection molded by any type of machinery on the market, provided that the plasticizing unit and the mold temperature control system have been configured appropriately. The machinery manufacturer must be consulted if any doubts exist on the ability of various parts to withstand the high temperatures required (e.g. barrel, barrel head, bolted connections, etc.)
Long residence time in combination with high temperatures should be avoided e.g. by pump out material at regular intervals.
During extended interruptions, the barrel temperature should be lowered to about 250-280°C.
It has been found out that heating to the requested processing temperature and shutting down or lowering the temperature is best carried out in two steps.
First, the barrel temperatures are set at the lower processing temperature range for the particular thermoplastic (340 - 350 °C). As soon as these temperatures have reached a steady state, the material in the barrel is pumped out. Second, the barrel temperature can be set to the required processing temperature or the heaters can be shut down.
Pre/Post-processing, max. allowed water content: .02 %
Pre/Post-processing, Pre-drying, Temperature: 140 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
injection molding, Melt temperature, range: 350 - 390 °C
injection molding, Melt temperature, recommended: 370 °C
injection molding, Mold temperature, range: 140 - 180 °C
injection molding, Mold temperature, recommended: 160 °C
Pretreatment
Drying temperature: 130 - 150°C
Drying time: minimum 4h
recommended dryer: vaccum or dry air dryer
maximum moisture: 0,02 - 0,05%
Ultrason® can be injection molded by any type of machinery on the market, provided that the plasticizing unit and the mold temperature control system have been configured appropriately. The machinery manufacturer must be consulted if any doubts exist on the ability of various parts to withstand the high temperatures required (e.g. barrel, barrel head, bolted connections, etc.)
Long residence time in combination with high temperatures should be avoided e.g. by pump out material at regular intervals.
During extended interruptions, the barrel temperature should be lowered to about 250-280°C.
It has been found out that heating to the requested processing temperature and shutting down or lowering the temperature is best carried out in two steps.
First, the barrel temperatures are set at the lower processing temperature range for the particular thermoplastic (340 - 350 °C). As soon as these temperatures have reached a steady state, the material in the barrel is pumped out. Second, the barrel temperature can be set to the required processing temperature or the heaters can be shut down.
Chemical Media Resistance
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.
In order to check the availability of products please contact us or our
sales agency.
For more information about our products contact your local BASF
representative or
BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail
CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.
In order to check the availability of products please contact us or our
sales agency.
For more information about our products contact your local BASF
representative or
BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail
CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991