This datasheet of Ultrason® KR 4113 from BASF is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Ultrason® KR 4113 | (PESU+PTFE)-(CF+CD)30... | BASF
Product Texts
Compound based on PES with 30 % filler. The filler system, a mixture of carbon fibres, graphite and PTFE powder, considerably improves Ultrason tribological properties. In addition, this product has a very small expansion coefficient and low tendency to swell in hot oils.
Abbreviated designation according to ISO 1043-1: PESU+ PTFE-(CF+CD)
Rheological propertiesdry / condUnitTest Standard
Melt volume-flow rate (MVR) 10 / * cm³/10min ISO 1133
Temperature 360 / * °C ISO 1133
Load 10 / * kg ISO 1133
Molding shrinkage (parallel) 0.3 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.5 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus - / 10100 MPa ISO 527-1/-2
Stress at break - / 105 MPa ISO 527-1/-2
Strain at break - / 1.3 % ISO 527-1/-2
Charpy impact strength (+23°C) - / 19 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) - / 4.5 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) * / 3 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Glass transition temperature (10°C/min) 225 / * °C ISO 11357-1/-2
Temp. of deflection under load (1.80 MPa) 220 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 225 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion (parallel) 11 / * E-6/K ISO 11359-1/-2
Electrical propertiesdry / condUnitTest Standard
Volume resistivity * / 8500 Ohm*m IEC 60093
Surface resistivity * / 4000 Ohm IEC 60093
Electric strength * / 8 kV/mm IEC 60243-1
Other propertiesdry / condUnitTest Standard
Water absorption 1.5 / * % Sim. to ISO 62
Humidity absorption 0.5 / * % Sim. to ISO 62
Density 1480 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
Viscosity number 56 / * cm³/g ISO 307, 1157, 1628
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 370 °C ISO 294
Injection Molding, mold temperature 170 °C ISO 10724
Injection Molding, injection velocity 200 mm/s ISO 294
Injection Molding, pressure at hold 80 MPa ISO 294
Diagrams
Dynamic Tensile modulus-temperature , Ultrason® KR 4113, (PESU+PTFE)-(CF+CD)30..., BASF
Stress-strain , Ultrason® KR 4113, (PESU+PTFE)-(CF+CD)30..., BASF
Secant modulus-strain , Ultrason® KR 4113, (PESU+PTFE)-(CF+CD)30..., BASF
Characteristics
Processing
Injection Molding, Sheet Extrusion
Delivery form
Pellets
Additives
Lubricants
Special Characteristics
Increased electrical conductivity, Anti-static
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .02 %
Pre/Post-processing, Pre-drying, Temperature: 140 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 350 - 390 °C
injection molding, Melt temperature, recommended: 370 °C
injection molding, Mold temperature, range: 150 - 190 °C
injection molding, Mold temperature, recommended: 170 °C

Pretreatment
Drying temperature: 130 - 150°C
Drying time: minimum 4h
recommended dryer: vaccum or dry air dryer
maximum moisture: 0,02 - 0,05%

Ultrason® can be injection molded by any type of machinery on the market, provided that the plasticizing unit and the mold temperature control system have been configured appropriately. The machinery manufacturer must be consulted if any doubts exist on the ability of various parts to withstand the high temperatures required (e.g. barrel, barrel head, bolted connections, etc.)

Long residence time in combination with high temperatures should be avoided e.g. by pump out material at regular intervals.
During extended interruptions, the barrel temperature should be lowered to about 250-280°C.

It has been found out that heating to the requested processing temperature and shutting down or lowering the temperature is best carried out in two steps.
First, the barrel temperatures are set at the lower processing temperature range for the particular thermoplastic (340 - 350 °C). As soon as these temperatures have reached a steady state, the material in the barrel is pumped out. Second, the barrel temperature can be set to the required processing temperature or the heaters can be shut down.
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact your local BASF
representative or

BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991