View list of
Sorting the List by Numerical Properties?
- All Evonik Degussa grades
- All PA66/6T grades
- All grades beginning with V
FREE DOWNLOAD
Interested inSorting the List by Numerical Properties?
The CAMPUS desktop version
offers extended functionality!CAMPUS® datasheet | VESTAMID HTplus M1036
This datasheet of VESTAMID HTplus M1036 from Evonik Industries AG is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
You may contact the supplier for more information about this grade.
VESTAMID® HTplus M1036 | PA66/6T-GF60 | Evonik Industries AG
Product Texts
VESTAMID® HTplus M1036
VESTAMID® HTplus M1036 is a glass-fiber reinforced (60%), heat-stabilized
polyphthalamide compound (PPA) for injection molding.
This compound is especially suitable for manufacting parts subjected to high
temperature.
VESTAMID® HTplus M1036 is supplied as cylindrical pellets in polyethylene
packaging.
For futher information, please contact our experts in the department Market
Development of the High Performance Polymers Business Line.
| Mechanical properties | dry / cond | Unit | Test Standard |
| Tensile Modulus | 23000 / - | MPa | ISO 527-1/-2 |
| Stress at break | 260 / - | MPa | ISO 527-1/-2 |
| Strain at break | 1.5 / - | % | ISO 527-1/-2 |
| Charpy impact strength (+23°C) | 60 / - | kJ/m² | ISO 179/1eU |
| Charpy impact strength (-30°C) | 40 / - | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 17 / - | kJ/m² | ISO 179/1eA |
| Charpy notched impact strength (-30°C) | 17 / - | kJ/m² | ISO 179/1eA |
| Thermal properties | dry / cond | Unit | Test Standard |
| Melting temperature (10°C/min) | 308 / * | °C | ISO 11357-1/-3 |
| Temp. of deflection under load (1.80 MPa) | 293 / * | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 305 / * | °C | ISO 75-1/-2 |
| Vicat softening temperature (50°C/h 50N) | 308 / * | °C | ISO 306 |
| Other properties | dry / cond | Unit | Test Standard |
| Water absorption | 3.2 / * | % | Sim. to ISO 62 |
| Humidity absorption | 0.2 / * | % | Sim. to ISO 62 |
| Density | 1770 / - | kg/m³ | ISO 1183 |
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
Drying at 120°C for at least 4 hours before processing is recommended.
For futher information, please contact our experts in the department Market
Development of the High Performance Polymers Business Line.
Disclaimer
With the following data, which reflect our current knowledge and experience, we wish to describe possible applications, however this information is given without guarantee or assurance of the appropriate properties for a specific application. The processor is not relieved of the responsibility for incoming quality control nor from his own testing and analysis. All data concerning product safety (EG-guideline, BGVV, FDA) are of principle nature and can be limitied regarding migration, temperature and type of food. They reflect the status as of Feb. 29, 2012. To insure that this data reflects the current state, please contact our Product Safety Department. Should you have any questions, wishes or suggestions about CAMPUS, please refer to the following address: Link to Evonik Industries AG homepage In any case, we hope you enjoy working with CAMPUS!
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991