Product Texts
VESTAMID® L-GF30 nc

 

Resin:                        ISO 1874-PA12, MHR, 18-070, GF30

 

Former Designation: VESTAMID® X4583 nc (t)

 

UL recognition:         UL 94:HB, NC, UL 746 B, RTI=120/105/105°C

 

Glass fibre reinforced (30%) PA12 resin for injection moulding.


Application examples: ball-bearing holders for windshield wiper arms

Rheological propertiesdry / condUnitTest Standard
Melt volume-flow rate (MVR) 30 / * cm³/10min ISO 1133
Temperature 275 / * °C ISO 1133
Load 5 / * kg ISO 1133
Molding shrinkage (parallel) 0.1 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.7 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 6500 / 5500 MPa ISO 527-1/-2
Yield stress * / 110 MPa ISO 527-1/-2
Yield strain * / 5 % ISO 527-1/-2
Nominal strain at break * / 5.5 % ISO 527-1/-2
Stress at break 120 / * MPa ISO 527-1/-2
Strain at break 5 / * % ISO 527-1/-2
Charpy impact strength (+23°C) 85 / 75 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 100 / 95 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 23 / 24 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 21 / 22 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 178 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 165 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 175 / * °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 175 / * °C ISO 306
Coeff. of linear therm. expansion (parallel) 60 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 70 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
UL recognition UL / * - -
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 3.2 / * mm IEC 60695-11-10
UL recognition UL / * - -
Electrical propertiesdry / condUnitTest Standard
Relative permittivity (100Hz) 4.1 / 5 - IEC 60250
Relative permittivity (1MHz) 3.4 / 4 - IEC 60250
Dissipation factor (100Hz) 310 / 600 E-4 IEC 60250
Dissipation factor (1MHz) 330 / 400 E-4 IEC 60250
Volume resistivity >1E13 / 2E12 Ohm*m IEC 60093
Surface resistivity * / >1E15 Ohm IEC 60093
Electric strength 44 / 45 kV/mm IEC 60243-1
Comparative tracking index 600 / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 1.1 / * % Sim. to ISO 62
Humidity absorption 0.5 / * % Sim. to ISO 62
Density 1240 / 1240 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1090 kg/m³ -
Thermal conductivity of melt 0.28 W/(m K) -
Spec. heat capacity melt 2400 J/(kg K) -
Ejection temperature 180 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 260 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Injection Molding, injection velocity 200 mm/s ISO 294
Injection Molding, pressure at hold 70 MPa ISO 294
Diagrams
Viscosity-shear rate , VESTAMID® L-GF30 nc (nf), PA12-GF30, Evonik Degussa
Shearstress-shear rate , VESTAMID® L-GF30 nc (nf), PA12-GF30, Evonik Degussa
Dynamic Shear modulus-temperature , VESTAMID® L-GF30 nc (nf), PA12-GF30, Evonik Degussa
Stress-strain , VESTAMID® L-GF30 nc (nf), PA12-GF30, Evonik Degussa
Secant modulus-strain , VESTAMID® L-GF30 nc (nf), PA12-GF30, Evonik Degussa
Stress-strain (isochronous) 23°C, VESTAMID® L-GF30 nc (nf), PA12-GF30, Evonik Degussa
Creep modulus-time 23°C, VESTAMID® L-GF30 nc (nf), PA12-GF30, Evonik Degussa
Tensile modulus-temperature , VESTAMID® L-GF30 nc (nf), PA12-GF30, Evonik Degussa
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PREPROCESSING INFORMATION
Maximum Water Content: 0.1 %
When the indicated water content is exceeded, the resin must be dried. The drying time is dependent

on the drying temperature. At a drying temperature of 80°C we recommend, depending on the water

content, a drying time of 8 - 16 hours. Fresh air dryers are acceptable, better would be a dry air or

vacuum dryer. Please note our product literature, plasticized resins can lose plasticizer during drying.


PROCESSING INFORMATION
Melt Temperature:240 - 280°C
Mold Temperature:30 - 100°C
Disclaimer
With the following data, which reflect our current knowledge and experience,
we wish to describe possible applications, however this information is given
without guarantee or assurance of the appropriate properties for a specific
application.

The processor is not relieved of the responsibility for incoming quality control
nor from his own testing and analysis.

All data concerning product safety (EG-guideline, BGVV, FDA) are of principle
nature and can be limitied regarding migration, temperature and type of food.
They reflect the status as of Feb. 29, 2012. To insure that this data reflects the
current state, please contact our Product Safety Department.

Should you have any questions, wishes or suggestions about CAMPUS,
please refer to the following address:

  Link to Evonik Industries AG homepage

In any case, we hope you enjoy working with CAMPUS!

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991