VESTODUR® GF30 nc


Resin:                        ISO 7792-PBT, MHR, A10-11, GF30

 

Former Designation: VESTODUR® SGF 30 nf

 

UL recognition: UL 94:HB; UL 746 B, RTI=130/130/140°C

 

Glass fibre reinforced (30%) PBT resin.

For the injection moulding of very rigid and heat resistant parts.

Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 13 cm³/10min ISO 1133
Temperature 250 °C ISO 1133
Load 2.16 kg ISO 1133
Molding shrinkage (parallel) 0.2 % ISO 294-4, 2577
Molding shrinkage (normal) 1.5 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 9500 MPa ISO 527-1/-2
Stress at break 160 MPa ISO 527-1/-2
Strain at break 3 % ISO 527-1/-2
Tensile creep modulus (1h) 9000 MPa ISO 899-1
Tensile creep modulus (1000h) 6500 MPa ISO 899-1
Charpy impact strength (+23°C) 75 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 80 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 12 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 12 kJ/m² ISO 179/1eA
Tensile notched impact strength (+23°C) 75 kJ/m² ISO 8256/1
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 223 °C ISO 11357-1/-3
Glass transition temperature (10°C/min) 45 °C ISO 11357-1/-2
Temp. of deflection under load (1.80 MPa) 210 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 223 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 213 °C ISO 306
Coeff. of linear therm. expansion (parallel) 50 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 60 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.6 mm IEC 60695-11-10
UL recognition UL - -
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm IEC 60695-11-10
UL recognition UL - -
Electrical propertiesValueUnitTest Standard
Relative permittivity (100Hz) 4 - IEC 60250
Relative permittivity (1MHz) 4.4 - IEC 60250
Dissipation factor (100Hz) 30 E-4 IEC 60250
Dissipation factor (1MHz) 170 E-4 IEC 60250
Volume resistivity >1E13 Ohm*m IEC 60093
Surface resistivity 1E14 Ohm IEC 60093
Electric strength 27 kV/mm IEC 60243-1
Comparative tracking index 450 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.5 % Sim. to ISO 62
Humidity absorption 0.5 % Sim. to ISO 62
Density 1530 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1370 kg/m³ -
Thermal conductivity of melt 0.28 W/(m K) -
Spec. heat capacity melt 1700 J/(kg K) -
Ejection temperature 220 °C -
Test specimen productionValueUnitTest Standard
Processing conditions acc. ISO 7790 - ISO ....-2
Injection Molding, melt temperature 260 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Injection Molding, injection velocity 200 mm/s ISO 294
Injection Molding, pressure at hold 70 MPa ISO 294
Diagrams
Viscosity-shear rate , VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Shearstress-shear rate , VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Dynamic Shear modulus-temperature , VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Stress-strain , VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Secant modulus-strain , VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Stress-strain (isochronous) 23°C, VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Creep modulus-time 23°C, VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Specific volume-temperature (pvT) , VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Tensile modulus-temperature , VESTODUR® GF30 nc (nf), PBT-GF30, Evonik Degussa
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Release agent
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding

PREPROCESSING INFORMATION
Maximum Water Content: 0.05 %
When the indicated water content is exceeded, the resin must be dried. The drying time is dependent

on the drying temperature. We recommend a drying time of approximately 5 hours at a temperature of

120°C in a fresh air dryer, better yet would be a dry air or vacuum dryer.


PROCESSING INFORMATION

Melt Temperature:240 - 280°C
Mold Temperature:50 - 120°C
Disclaimer
With the following data, which reflect our current knowledge and experience,
we wish to describe possible applications, however this information is given
without guarantee or assurance of the appropriate properties for a specific
application.

The processor is not relieved of the responsibility for incoming quality control
nor from his own testing and analysis.

All data concerning product safety (EG-guideline, BGVV, FDA) are of principle
nature and can be limitied regarding migration, temperature and type of food.
They reflect the status as of Feb. 29, 2012. To insure that this data reflects the
current state, please contact our Product Safety Department.

Should you have any questions, wishes or suggestions about CAMPUS,
please refer to the following address:

  Link to Evonik Industries AG homepage

In any case, we hope you enjoy working with CAMPUS!