  Zytel® ST800HSL BK152 | PA66-I | DuPont Engineering Polymers
Product Texts
Common features of Zytel® nylon resin include mechanical and physical properties such as high mechanical strength, excellent balance of stiffness and toughness, good high temperature performance, good electrical and flammability properties, good abrasion and chemical resistance.

In addition, Zytel® nylon resins are available in different modified and reinforced grades to create a wide range of products with tailored properties for specific processes and end-uses. Zytel® nylon resin, including most flame retardant grades, offer the ability to be coloured.

The good melt stability of Zytel® nylon resin normally enables the recycling of properly handled production waste. If recycling is not possible, DuPont recommends, as the preferred option, incineration with energy recovery (-31kJ/g of base polymer) in appropriately equipped installations. For disposal, local regulations have to be observed.

Zytel® nylon resin typically is used in demanding applications in the automotive, furniture, domestic appliances, sporting goods and construction industry.

______________________________________________________


Zytel® ST800HSL is an unreinforced, heat stabilized, lubricated and super tough polyamide 66 for injection molding. It provides outstanding impact resistance, improved production cycles and and is specifically suitable for laser marking.

Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 1.8 / * % ISO 294-4, 2577
Molding shrinkage (normal) 1.8 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 2000 / - MPa ISO 527-1/-2
Yield stress 51 / - MPa ISO 527-1/-2
Yield strain 6 / - % ISO 527-1/-2
Nominal strain at break 38 / - % ISO 527-1/-2
Charpy impact strength (+23°C) N / - kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 72 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 263 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 61 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion (parallel) 110 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 120 / * E-6/K ISO 11359-1/-2
Other propertiesdry / condUnitTest Standard
Density 1090 / - kg/m³ ISO 1183
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PREPROCESSING
Drying Recommended = Yes, if moisture content of resin exceeds recommended level
Drying Temperature = 80°C
Drying Time, Dehumidified Dryer = 2-4h
Processing Moisture Content = <0.2 %
PROCESSING
Melt Temperature Optimum = 290°C
Melt Temperature Range = 280-300°C
Mold Temperature Optimum = 70°C
Mold Temperature Range = 50-90°C
Maximum Screw tangential Speed : 0.3 m/s
Flow front speed : 150 mm/s
Hold pressure optimum : 85 MP a
Hold pressure range : 50-100 MPa
Back pressure : low
Hold pressure time : 3 s/mm
Maximum hold-up time : 10 min
Moulding guide
Chemical Media Resistance
Disclaimer

E.I. du Pont de Nemours and Company is pleased to provide information about its products with the CAMPUS electronic database.

The information provided is gratis and DuPont assumes no obligation or liability for any advice furnished or for any results obtained with respect to this information.

All such advice is given and accepted at the risk of the buyer. The disclosure of information herein is not an express or implied license to operate under any patent of DuPont or others.

DuPont warrants that the use or sale of any material which is described herein and is offered for sale by DuPont does not infringe any patent covering the material itself, but does not warrant against infringement by reason of the use thereof in combination with other materials or the operation of any process.

Unless otherwise noted, the property values are for natural color (NC010) resins only. Colorants or other additives may alter some or all of the properties.
The data listed herein fall within the normal range of product properties and they should not be used to establish specification limits nor used alone as the basis of design.

Material Safety Data Sheets (SDSs) can be obtained from local sales offices.

Products listed herein should not be used in medical applications involving permanent implantation in the human body or contact with internal body fluids or tissues unless the material has been provided from DuPont under a written contract that is consistent with DuPont policy regarding medical applications and expressly acknowledges the contemplated use.

For further information, please contact your DuPont representative.

You may also request a copy of DuPont policy regarding medical applications H-50103-2 and DuPont caution regarding medical applications H-50102-2.

Products listed herein may from time to time be modified or removed.
Please call your local sales office to determine current availability.


The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991