Texto del producto
  • MVR (300 °C/1.2 kg) 14 cm3/10 min
  • medical devices
  • suitable for ETO and steam sterilization at 121 °C
  • biocompatible according to many ISO 10993-1 test requirements
  • medium viscosity
  • easy release
  • available in transparent and opaque colors
Propiedades reológicasValorUnidadesMétodo de ensayo
Indice de fluidez volumétrico, MVR 14 cm³/10min ISO 1133
Temperatura 300 °C ISO 1133
Carga 1.2 kg ISO 1133
Contracción posterior al moldeo, paralelo 0.7 % ISO 294-4, 2577
Contracción posterior al moldeo, normal 0.7 % ISO 294-4, 2577
Propiedades mecánicasValorUnidadesMétodo de ensayo
Módulo de tracción 2400 MPa ISO 527-1/-2
Esfuerzo de fluencia 66 MPa ISO 527-1/-2
Alarg. en límite elástico 6.1 % ISO 527-1/-2
Alarg. nominal a rotura >50 % ISO 527-1/-2
Módulo de plastodeformación, 1h 2200 MPa ISO 899-1
Módulo de plastodeformación, 1000h 1900 MPa ISO 899-1
Resistencia al impacto Charpy, +23°C N kJ/m² ISO 179/1eU
Resistencia al impacto Charpy, -30°C N kJ/m² ISO 179/1eU
Perforación - máxima fuerza, +23°C 5400 N ISO 6603-2
Perforación - máxima fuerza, -30°C 6300 N ISO 6603-2
Perforación - energía, +23°C 60 J ISO 6603-2
Perforación - energía, -30°C 65 J ISO 6603-2
Propiedades térmicasValorUnidadesMétodo de ensayo
Temp. de transición vítrea, 10°C/min 144 °C ISO 11357-1/-2
Estabilidad al calor, 1.80 MPa 124 °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 136 °C ISO 75-1/-2
Temp. reblandecimiento Vicat, 50°C/h 50N 144 °C ISO 306
Coef.de expansión térmica lineal, paralelo 65 E-6/K ISO 11359-1/-2
Coef.de expansión térmica lineal, normal 65 E-6/K ISO 11359-1/-2
Combustibilidad a 1.5mm esp. nom. V-2 class IEC 60695-11-10
Espesores de probeta 1.5 mm IEC 60695-11-10
Valoración UL UL - -
Combustibilidad a espesor h HB class IEC 60695-11-10
Espesores de probeta 2.5 mm IEC 60695-11-10
Valoración UL UL - -
Combustibilidad según índice de oxigeno 28 % ISO 4589-1/-2
Propiedades eléctricasValorUnidadesMétodo de ensayo
Constante dieléctrica, 100Hz 3.1 - IEC 60250
Constante dieléctrica, 1MHz 3 - IEC 60250
Factor de pérdidas dieléctricas, 100Hz 5 E-4 IEC 60250
Factor de pérdidas dieléctricas, 1MHz 90 E-4 IEC 60250
Resistividad volumétrica específica >1E13 Ohm*m IEC 60093
Resistividad superficial específica >1E15 Ohm IEC 60093
Resistencia dieléctrica 34 kV/mm IEC 60243-1
Indice comparativo de linea de fuga 250 - IEC 60112
Otras propiedadesValorUnidadesMétodo de ensayo
Absorción de agua 0.3 % Sim. to ISO 62
Absorción de humedad 0.12 % Sim. to ISO 62
Densidad 1200 kg/m³ ISO 1183
Propiedades específicas del materialValorUnidadesMétodo de ensayo
Transmitancia luminosa 89 % ISO 13468-1, -2
Cálculo propiedades reológicasValorUnidadesMétodo de ensayo
Densidad de fusión 1020 kg/m³ -
Conductibilidad termica de fusión 0.214 W/(m K) -
Calor especifico de la masa 2100 J/(kg K) -
Difusibidad termica 1E-7 m²/s -
Temperatura de expulsión 130 °C -
Condiciones de transformaciónValorUnidadesMétodo de ensayo
Moldeo por inyección, temperatura de la masa 290 °C ISO 294
Moldeo por inyección, temperatura del molde 80 °C ISO 10724
Moldeo por inyección, velocidad de inyección 200 mm/s ISO 294
Funciones
Viscosidad-velocidad de cizallamiento , Makrolon® 2558, PC, Bayer MatSc
Tensión de cizalla-velocidad de cizalla , Makrolon® 2558, PC, Bayer MatSc
Módulo de cizallamiento dinámico-temperatura , Makrolon® 2558, PC, Bayer MatSc
Esfuerzo-alargamiento , Makrolon® 2558, PC, Bayer MatSc
Módulo secante-alargamiento , Makrolon® 2558, PC, Bayer MatSc
Esfuerzo-alargamiento (isocrono) 23°C, Makrolon® 2558, PC, Bayer MatSc
Módulo de plastodeformación-tiempo 23°C, Makrolon® 2558, PC, Bayer MatSc
Esfuerzo-alargamiento (isocrono) 40°C, Makrolon® 2558, PC, Bayer MatSc
Módulo de plastodeformación-tiempo 40°C, Makrolon® 2558, PC, Bayer MatSc
Esfuerzo-alargamiento (isocrono) 60°C, Makrolon® 2558, PC, Bayer MatSc
Módulo de plastodeformación-tiempo 60°C, Makrolon® 2558, PC, Bayer MatSc
Esfuerzo-alargamiento (isocrono) 90°C, Makrolon® 2558, PC, Bayer MatSc
Módulo de plastodeformación-tiempo 90°C, Makrolon® 2558, PC, Bayer MatSc
Esfuerzo-alargamiento (isocrono) 120°C, Makrolon® 2558, PC, Bayer MatSc
Módulo de plastodeformación-tiempo 120°C, Makrolon® 2558, PC, Bayer MatSc
Volumen especifico-temperatura (pvT) , Makrolon® 2558, PC, Bayer MatSc
Características
Procesamiento y forma de entrega
Moldeo por inyección
Forma de suministro
Sémola
Aditivos
Desmoldeante
Características especiales
Transparente
Disponibilidad regional
Aviso

Bayer MaterialScience AG

The manner in which you use and the purpose to which you put and utilize our products, technical assistance and information (whether verbal, written or by way of production evaluations), including any suggested formulations and recommendations, are beyond our control. Therefore, it is imperative that you test our products, technical assistance and information to determine to your own satisfaction whether they are suitable for your intended uses and applications. This application-specific analysis must at least include testing to determine suitability from a technical as well as health, safety and environmental standpoint. Such testing has not necessarily been done by us. Unless we otherwise agree in writing, all products are sold strictly pursuant to the terms of our standard conditions of sale which are available upon request. All information and technical assistance is given without warranty or guarantee, and is subject to change without notice. It is expressly understood and agreed that you assume and hereby expressly release us from all liability, in tort, contract or otherwise, incurred in connection with the use of our products, technical assistance and information. Any statement or recommendation not contained herein is unauthorized and shall not bind us. Nothing herein shall be construed as a recommendation to use any product in conflict with patents covering any material or its use. No license is implied or in fact granted under the claims of any patent. Unless specified to the contrary, the property values given have been established on standardized test specimens at room temperature. The figures should be regarded as typical values only and not as binding limiting values. Please note that the properties can be affected by the design of the mold/die, the processing conditions and coloring. With respect to health, safety and environment precautions, the relevant Material Safety Data Sheets (MSDS) and product labels must be observed prior to working with our products.


BMS Medical Grades

BMS Products that are designated as "Medical Grade", e.g., plastics, sheets, and films, meet certain biocompatibility test requirements of ISO Standard 10993-1: "Biological Evaluation of Medical Devices" for the categories including: 1) skin contact, 2) up to 24 hours contact with circulating blood, tissue, bone, and dentin, 3) up to 30 days contact with mucosal membranes, compromised surfaces, and blood path, indirect. BMS Products designated as "Medical Grade" shall not be considered candidates for the following types of Medical Applications unless BMS explicitly agrees, in writing, to sell such products for such applications: a) cosmetic, reconstructive, or reproductive implant applications; b) any other bodily implant applications; c)applications involving contact with or storage of human tissue, blood, or other bodily fluids, for greater than 30 days; or d) applications having greater than 24 hours contact with circulating blood, tissue, bone and dentin. The biocompatibility testing referenced above cannot assure the biocompatibility of final or intermediate products made from BMS Products or the suitability of such products for their use in a Medical Application, i.e., the test data cannot be used to conclude that any medical devices manufactured from the BMS Products meet the necessary requirements of ISO Standard 10993-1. It is the sole responsibility of the manufacturer of final end-use product to conduct all necessary tests (including biocompatibility tests) and inspections and to evaluate the final product under actual end-use requirements. The designation as "Medical Grade" does not mean that BMS or anyone else has determined that the product is suitable for use in any particular Medical Application. BMS makes no representations regarding the suitability of a BMS Product for a particular Medical Application or final enduse product. A determination that the BMS Product is suitable for use in a particular Medical Application or final end-use product can only be made by the purchaser of the BMS product who utilizes it in a Medical Application and conducts all necessary testing and evaluation to support such a determination.


Appropriate Use of BMS Products in a Medical Application

BMS has not performed clinical medical studies concerning the use of BMS Products. Moreover, BMS has neither sought nor received approval from the United States Food and Drug Administration (FDA) or other competent authorities from other regions for the use of BMS Products in a Medical Application. BMS makes no representations or warranty regarding (and accepts no responsibility for determining) either: (a) the suitability of a BMS Product for a particular Medical Application or final end-use product or (b) the adequacy of any warning relating to a BMS Product or particular Medical Application or final end-use product. The suitability of BMS Products in a given end-use environment is dependent upon various conditions including, without limitation, chemical compatibility, method of manufacture, temperature, part design, sterilization method, residual stresses, and external loads. It is the sole responsibility of the manufacturer of the final end-use product to determine the suitability (including biocompatibility) of all raw materials and components, including any BMS Products, in order to ensure that the final product: - meets relevant biocompatibility requirements and is otherwise safe for its end-use, - performs or functions as intended, - is suitable for its intended use, and - complies with all applicable FDA and other regulatory requirements. It also is the sole responsibility of the manufacturer of the final end-use product to conduct all necessary tests and inspections and to evaluate the final product under actual end-use requirements and to adequately advise and warn purchasers, users, and/or learned intermediaries (such as physicians) of pertinent risks and fulfill any postmarket surveillance obligations. Any decision regarding the appropriateness of a particular medical product in a particular clinical or Medical Application should be based on the judgment of the manufacturer, seller, the competent authority, and the treating physician. BMS cannot weigh the benefits against the risks of a medical device and cannot offer a medical or legal judgment on the safety or efficacy of the use of a BMS Product in a specific Medical Application. Terms in capital letters as used herein shall have the same meaning as defined in the "GUIDANCE ON USE OF BAYER MATERIALSCIENCE PRODUCTS IN A MEDICAL APPLICATION" which can be found under (see here). It is the customer's responsibility to thoroughly review the Guidance Document in detail and to diligently consider its content prior to any use of BMS Products in Medical Applications. For further information on our Medical Grades please see our brochure "Makrolon, Apec and Bayblend for medical devices".

www.bayerplastics.com

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012