CAMPUS® datasheet | Grivory XE 3858 black 9915
This datasheet of Grivory XE 3858 black 9915 from EMS-GRIVORY | a unit of EMS-CHEMIE AG is provided by the international plastics database CAMPUS.
You may contact the supplier for more information about this grade.
Grivory XE 3858 black 9915 | PA*-GF50 | EMS-GRIVORY - a unit of EMS-CHEMIE AG
Informations produit
Product designation according to ISO 1874:
PA66/6I/X, MH, 11-160, GF50
Partially aromatic Polyamide
Product Attributes
| Improved flowability and demoulding, Improved UV resistance (outdoor use) |
Markets
| Automotive | |
| Air intake sytems, Automotive electr. and electronics, lighting, Cooling and climate control, Powertrain and Chassis , Interior, Exterior | |
| Electricals & Electronics | |
| Electrical appliances, Electrical equipment, Connectors, Energy distribution, Mobile phones and other portable devices | |
| Industry & Consumer goods | |
| Housewares, Mechanical Engineering, Sanitary, water and gas supply, Tools & Accessories |
| Propriétés rhéologiques | sec / cond | Unité | Norme du test |
| Retrait au moulage, parallèle | 0.1 / * | % | ISO 294-4, 2577 |
| Retrait au moulage, perpendiculaire | 0.4 / * | % | ISO 294-4, 2577 |
| Propriétés mécaniques | sec / cond | Unité | Norme du test |
| Module en traction | 16500 / 16500 | MPa | ISO 527-1/-2 |
| Contrainte à la rupture | 230 / 200 | MPa | ISO 527-1/-2 |
| Déformation à la rupture | 2 / 2.5 | % | ISO 527-1/-2 |
| Résistance au choc Charpy, +23°C | 75 / 75 | kJ/m² | ISO 179/1eU |
| Résistance au choc Charpy, -30°C | 60 / 50 | kJ/m² | ISO 179/1eU |
| Résistance au choc Charpy (entaillé), +23°C | 15 / 14 | kJ/m² | ISO 179/1eA |
| Résistance au choc Charpy (entaillé), -30°C | 15 / 14 | kJ/m² | ISO 179/1eA |
| Propriétés thermiques | sec / cond | Unité | Norme du test |
| Température de fusion, 10°C/min | 235 / * | °C | ISO 11357-1/-3 |
| Température de fléchissement s/chrg, 1.80 MPa | 215 / * | °C | ISO 75-1/-2 |
| Température de fléchissement s/chrg, 8.00 MPa | 165 / * | °C | ISO 75-1/-2 |
| Coeffic. de dilatation therm. linéique, parallèle | 10 / * | E-6/K | ISO 11359-1/-2 |
| Coeffic. de dilatation therm. linéique, perpend. | 60 / * | E-6/K | ISO 11359-1/-2 |
| Inflammabilité pr. épaisseur h | HB / * | class | IEC 60695-11-10 |
| Epaisseur de l'éprouvette | 0.8 / * | mm | IEC 60695-11-10 |
| Propriétés électriques | sec / cond | Unité | Norme du test |
| Résistivité transversale | 1E10 / 1E11 | Ohm*m | IEC 60093 |
| Résistivité superficielle | * / 1E12 | Ohm | IEC 60093 |
| Rigidité diélectrique | 35 / 35 | kV/mm | IEC 60243-1 |
| Indice de résistance au cheminement | - / 600 | - | IEC 60112 |
| Propriétés diverses | sec / cond | Unité | Norme du test |
| Absorption d'eau | 4 / * | % | Sim. to ISO 62 |
| Absorption d'humidité | 1.4 / * | % | Sim. to ISO 62 |
| Masse volumique | 1590 / - | kg/m³ | ISO 1183 |
Caractéristiques
Transformation
Moulage par injection
Conditionnement
Granulés
Propriétés spéciales
Stabilisé aux intempéries
Disponibilité régionale
Conditions générales
EMS-CHEMIE AG Business Unit EMS-GRIVORY Homepage : EMS-GRIVORY eMail : welcome@emsgrivory.com The values are intended to serve as an aid in preselecting materials and for an overview of the EMS-GRIVORY product range. The information contained in this publication is based on our present knowledge and experience. The given figures and data are guidance values and do not represent binding material specifications. No warranties of any kind, either express or implied, including warranties of merchantability or fitness for a particular purpose, are given regarding products, design, data and information. The customer is not released from his obligation to investigate the products fitness and the suitability for the intended application, compliance with legal requirements and intellectual property rights. We reserve the right to change the information at any time and without prior notice. The information in this publication is not to be considered a contractual obligation and any liability whatsoever is expressly declined. For further questions about our products please contact our experts.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.