View list of
CAMPUS® datasheet | CELANEX 4305
This datasheet of CELANEX 4305 from Ticona is provided by the international plastics database CAMPUS.
You may contact the supplier for more information about this grade.
CELANEX 4305 | PBT-GF33 | Ticona
商品の説明文
Celanex 4305 is a 33% glass reinforced, toughened, thermoplastic
polyester.
polyester.
| レオロジー特性 | 値 | 単位 | テスト基準 |
| メルトボリュームレイト, MVR | 5.7 | cm³/10min | ISO 1133 |
| 温度 | 250 | °C | ISO 1133 |
| 荷重 | 2.16 | kg | ISO 1133 |
| 機械的特性 | 値 | 単位 | テスト基準 |
| 引張弾性率 | 9500 | MPa | ISO 527-1/-2 |
| 破壊応力 | 110 | MPa | ISO 527-1/-2 |
| 破壊ひずみ | 3 | % | ISO 527-1/-2 |
| シャルピー衝撃強さ, +23°C | 54 | kJ/m² | ISO 179/1eU |
| シャルピー衝撃強さ, -30°C | 54 | kJ/m² | ISO 179/1eU |
| ノッチ付きシャルピー衝撃強さ, +23°C | 13.1 | kJ/m² | ISO 179/1eA |
| ノッチ付きシャルピー衝撃強さ, -30°C | 13.2 | kJ/m² | ISO 179/1eA |
| 熱的特性 | 値 | 単位 | テスト基準 |
| 溶融温度, 10°C/min | 225 | °C | ISO 11357-1/-3 |
| 荷重たわみ温度, 1.80 MPa | 206 | °C | ISO 75-1/-2 |
| 荷重たわみ温度, 0.45 MPa | 224 | °C | ISO 75-1/-2 |
| 線膨張係数, 平行 | 20 | E-6/K | ISO 11359-1/-2 |
| 線膨張係数, 直角 | 65 | E-6/K | ISO 11359-1/-2 |
| 試験片の成形条件. | 値 | 単位 | テスト基準 |
| ISO規格による成形条件 | 7790 | - | ISO ....-2 |
| 射出成形, 樹脂温度 | 260 | °C | ISO 294 |
| 射出成形, 金型温度 | 82 | °C | ISO 10724 |
| 射出成形, 射出速度 | 300 | mm/s | ISO 294 |
| 射出成形, 保圧 | 48 | MPa | ISO 294 |
Disclaimer
NOTICE TO USERS: Values shown are based on testing of laboratory test specimens and represent data that fall within the standard range of properties for natural material. These values alone do not represent a sufficient basis for any part design and are not intended for use in establishing maximum, minimum, or ranges of values for specification purposes. Colorants or other additives may cause significant variations in data values. Properties of molded parts can be influenced by a wide variety of factors including, but not limited to, material selection, additives, part design, processing conditions and environmental exposure. Any determination of the suitability of a particular material and part design for any use contemplated by the users and the manner of such use is the sole responsibility of the users, who must assure themselves that the material as subsequently processed meets the needs of their particular product or use. To the best of our knowledge, the information contained in this publication is accurate; however, we do not assume any liability whatsoever for the accuracy and completeness of such information. The information contained in this publication should not be construed as a promise or guarantee of specific properties of our products. It is the sole responsibility of the users to investigate whether any existing patents are infringed by the use of the materials mentioned in this publication. Moreover, there is a need to reduce human exposure to many materials to the lowest practical limits in view of possible adverse effects. To the extent that any hazards may have been mentioned in this publication, we neither suggest nor guarantee that such hazards are the only ones which exist. We recommend that persons intending to rely on any recommendation or to use any equipment, processing technique, or material mentioned in this publication should satisfy themselves that they can meet all applicable safety and health standards. We strongly recommend that users seek and adhere to the manufacturer's current instructions for handling each material they use, and to entrust the handling of such material to adequately trained personnel only. Please call the telephone numbers listed for additional technical information. Call Customer Services for the appropriate Materials Safety Data Sheets (MSDS) before attempting to process our products. The products mentioned herein are not intended for use in medical or dental implants.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012