Durethan® A 30 H3.0 | PA66 | LANXESS Deutschland GmbH
商品の説明文
PA 66, non-reinforced, injection moulding, heat-ageing stabilized
| 機械的特性 | 乾燥/調湿 | 単位 | テスト基準 |
| 引張弾性率 | 3500 / 1300 | MPa | ISO 527-1/-2 |
| 降伏応力 | 95 / 55 | MPa | ISO 527-1/-2 |
| 降伏ひずみ | 4.5 / 20 | % | ISO 527-1/-2 |
| 破壊呼びひずみ | - / >50 | % | ISO 527-1/-2 |
| シャルピー衝撃強さ, +23°C | 160 / 190 | kJ/m² | ISO 179/1eU |
| シャルピー衝撃強さ, -30°C | 100 / 100 | kJ/m² | ISO 179/1eU |
| ノッチ付きシャルピー衝撃強さ, +23°C | 10 / 20 | kJ/m² | ISO 179/1eA |
| ノッチ付きシャルピー衝撃強さ, -30°C | 10 / 10 | kJ/m² | ISO 179/1eA |
| 熱的特性 | 乾燥/調湿 | 単位 | テスト基準 |
| 溶融温度, 10°C/min | 261 / * | °C | ISO 11357-1/-3 |
| 荷重たわみ温度, 1.80 MPa | 70 / * | °C | ISO 75-1/-2 |
| 荷重たわみ温度, 0.45 MPa | 200 / * | °C | ISO 75-1/-2 |
| 線膨張係数, 平行 | 60 / * | E-6/K | ISO 11359-1/-2 |
| 線膨張係数, 直角 | 100 / * | E-6/K | ISO 11359-1/-2 |
| 電気的特性. | 乾燥/調湿 | 単位 | テスト基準 |
| 比誘電率, 100Hz | 3.8 / 13 | - | IEC 60250 |
| 比誘電率, 1MHz | 3.4 / 4.1 | - | IEC 60250 |
| 誘電正接, 100Hz | 120 / 3200 | E-4 | IEC 60250 |
| 誘電正接, 1MHz | 570 / 1000 | E-4 | IEC 60250 |
| 体積抵抗率 | >1E13 / 1E10 | Ohm*m | IEC 60093 |
| 表面抵抗率 | * / 1E13 | Ohm | IEC 60093 |
| 耐電圧 | 31 / 25 | kV/mm | IEC 60243-1 |
| 耐トラッキング性 | 600 / - | - | IEC 60112 |
| 流動解析用データ | 値 | 単位 | テスト基準 |
| 溶融時の密度 | 970 | kg/m³ | - |
| 溶融時の熱伝導率 | 0.225 | W/(m K) | - |
| 溶融時の比熱 | 2900 | J/(kg K) | - |
| 熱拡散率 | 8E-8 | m²/s | - |
| 突き出し時の時の温度 | 185 | °C | - |
| 試験片の成形条件. | 値 | 単位 | テスト基準 |
| 射出成形, 樹脂温度 | 280 | °C | ISO 294 |
| 射出成形, 金型温度 | 80 | °C | ISO 10724 |
Disclaimer
This information and our technical advice - whether verbal, in writing or by way of trials - are given in good faith but without warranty, and this also applies where proprietary rights of third parties are involved. Our advice does not release you from the obligation to check its validity and to test our products as to their suitability for the intended processes and uses. The application, use and processing of our products and the products manufactured by you on the basis of our technical advice are beyond our control and, therefore, entirely your own responsibility. Our products are sold in accordance with our General Conditions of Sale and Delivery. The values stored in the databank should only be used as guidelines for component design. In giving these values neither guarantee, nor assurance of particular material properties can be given. techcenter.lanxess.com
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012