レオロジー特性単位テスト基準
メルトボリュームレイト, MVR 7 cm³/10min ISO 1133
温度 220 °C ISO 1133
荷重 10 kg ISO 1133
機械的特性単位テスト基準
引張弾性率 3800 MPa ISO 527-1/-2
破壊応力 79 MPa ISO 527-1/-2
破壊ひずみ 3 % ISO 527-1/-2
引張クリープ弾性率, 1h 3500 MPa ISO 899-1
引張クリープ弾性率, 1000h 2800 MPa ISO 899-1
シャルピー衝撃強さ, +23°C 21 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 19 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 2.5 kJ/m² ISO 179/1eA
熱的特性単位テスト基準
荷重たわみ温度, 1.80 MPa 90 °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 102 °C ISO 75-1/-2
ビカット軟化温度, 50°C/h 50N 107 °C ISO 306
線膨張係数, 平行 70 E-6/K ISO 11359-1/-2
1.5mm厚さでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 1.6 mm IEC 60695-11-10
UL認定 UL - -
厚さhでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 0.8 mm IEC 60695-11-10
UL認定 UL - -
酸素指数 18 % ISO 4589-1/-2
電気的特性.単位テスト基準
比誘電率, 100Hz 3 - IEC 60250
比誘電率, 1MHz 2.8 - IEC 60250
誘電正接, 100Hz 50 E-4 IEC 60250
誘電正接, 1MHz 80 E-4 IEC 60250
体積抵抗率 >1E13 Ohm*m IEC 60093
表面抵抗率 >1E15 Ohm IEC 60093
耐トラッキング性 475 - IEC 60112
その他の特性.単位テスト基準
吸湿率 0.3 % Sim. to ISO 62
密度 1080 kg/m³ ISO 1183
流動解析用データ単位テスト基準
溶融時の密度 970 kg/m³ -
溶融時の熱伝導率 0.17 W/(m K) -
溶融時の比熱 2300 J/(kg K) -
突き出し時の時の温度 99 °C -
試験片の成形条件.単位テスト基準
射出成形, 樹脂温度 250 °C ISO 294
射出成形, 金型温度 60 °C ISO 10724
射出成形, 射出速度 200 mm/s ISO 294
機能
 粘度せん断速度. , Luran® 33100, SAN, Styrolution
 せん断応力-せん断速度. , Luran® 33100, SAN, Styrolution
 応力-ひずみ. , Luran® 33100, SAN, Styrolution
 割線弾性率−ひずみ. , Luran® 33100, SAN, Styrolution
 応力-ひずみ (等時的). 23°C, Luran® 33100, SAN, Styrolution
 クリープ弾性率−時間. 23°C, Luran® 33100, SAN, Styrolution
 応力-ひずみ (等時的). 40°C, Luran® 33100, SAN, Styrolution
 クリープ弾性率−時間. 40°C, Luran® 33100, SAN, Styrolution
 応力-ひずみ (等時的). 60°C, Luran® 33100, SAN, Styrolution
 クリープ弾性率−時間. 60°C, Luran® 33100, SAN, Styrolution
 応力-ひずみ (等時的). 80°C, Luran® 33100, SAN, Styrolution
 クリープ弾性率−時間. 80°C, Luran® 33100, SAN, Styrolution
 pvT , Luran® 33100, SAN, Styrolution
 引張弾性率-温度. , Luran® 33100, SAN, Styrolution
特殊な特性
成形加工法.
射出成形., 異形押出成形., シート押出成形., その他の押出成形., 熱成形.
納入形状.
ペレット.
特殊な特性.
透明.
領域別の利用可能性
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact

Styrolution GmbH
Styrolution Infopoint
mailto:styrenics.infopoint@basf.com
Tel: +49 621 60 41446

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012