SCHULAMID® 6 GB 30 | PA6-GB30 | A. Schulman GmbH
商品の説明文
30% glass bead reinforced PA 6 with increased stiffness and dimensional stability
| 機械的特性 | 乾燥/調湿 | 単位 | テスト基準 |
| 引張弾性率 | 4500 / 1800 | MPa | ISO 527-1/-2 |
| 破壊応力 | 80 / 50 | MPa | ISO 527-1/-2 |
| 破壊ひずみ | 8 / 12 | % | ISO 527-1/-2 |
| シャルピー衝撃強さ, +23°C | 30 / 45 | kJ/m² | ISO 179/1eU |
| シャルピー衝撃強さ, -30°C | 28 / 35 | kJ/m² | ISO 179/1eU |
| ノッチ付きシャルピー衝撃強さ, +23°C | 6 / 14 | kJ/m² | ISO 179/1eA |
| ノッチ付きシャルピー衝撃強さ, -30°C | 4 / 4 | kJ/m² | ISO 179/1eA |
| 熱的特性 | 乾燥/調湿 | 単位 | テスト基準 |
| 溶融温度, 10°C/min | 221 / * | °C | ISO 11357-1/-3 |
| ガラス転移点, 10°C/min | 42 / * | °C | ISO 11357-1/-2 |
| 荷重たわみ温度, 1.80 MPa | 70 / * | °C | ISO 75-1/-2 |
| 荷重たわみ温度, 0.45 MPa | 180 / * | °C | ISO 75-1/-2 |
| ビカット軟化温度, 50°C/h 50N | 200 / * | °C | ISO 306 |
| 1.5mm厚さでの燃焼性 | HB / * | class | IEC 60695-11-10 |
| 試験片の厚さ | 1.5 / * | mm | IEC 60695-11-10 |
| UL認定 | UL / * | - | - |
| 電気的特性. | 乾燥/調湿 | 単位 | テスト基準 |
| 比誘電率, 100Hz | 4 / 4 | - | IEC 60250 |
| 比誘電率, 1MHz | 4 / 4 | - | IEC 60250 |
| 誘電正接, 100Hz | 0.005 / 0.005 | E-4 | IEC 60250 |
| 誘電正接, 1MHz | 0.016 / 0.016 | E-4 | IEC 60250 |
| 体積抵抗率 | >1E13 / 1E10 | Ohm*m | IEC 60093 |
| 表面抵抗率 | * / >1E15 | Ohm | IEC 60093 |
| 耐トラッキング性 | - / 450 | - | IEC 60112 |
| 材料特有の特性 | 乾燥/調湿 | 単位 | テスト基準 |
| 粘度数 | 145 / * | cm³/g | ISO 307, 1157, 1628 |
| 流動解析用データ | 値 | 単位 | テスト基準 |
| 溶融時の密度 | 1250 | kg/m³ | - |
| 溶融時の熱伝導率 | 0.25 | W/(m K) | - |
| 熱拡散率 | 8E-8 | m²/s | - |
| 突き出し時の時の温度 | 110 | °C | - |
| 試験片の成形条件. | 値 | 単位 | テスト基準 |
| ISO規格による成形条件 | 1870 | - | ISO ....-2 |
| 射出成形, 樹脂温度 | 250 | °C | ISO 294 |
| 射出成形, 金型温度 | 80 | °C | ISO 10724 |
| 射出成形, 射出速度 | 250 | mm/s | ISO 294 |
| 射出成形, 保圧 | 70 | MPa | ISO 294 |
機能
Disclaimer
The information and recommendations contained in this document are based upon
data collected by A. Schulman and are believed to be reliable; however, because
A. Schulman cannot anticipate or control the many different conditions under
which this information and/or product may be used, no representation is made
and no warranty is given of any kind, express or implied, for completeness,
accuracy, availability, suitability, usefulness, commercial value, or non-violation
of intellectual property rights of information, recommendations, and products
and services directly or indirectly provided. A. Schulman assumes no responsibility
for the results of the use of products and processes described herein and expressly
disclaims the implied warranties of merchantability and fitness for a particular use
If there are questions to given information, to further properties or further A. Schulman
products please contact
A. Schulman GmbH
Huettenstrasse 211
50170 Kerpen
Tel: 02273 / 561-0
Contact: aschulman@de.aschulman.com
Subject: Material data
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012