CAMPUS® datasheet | Zytel® 70G43HSLA BK099


This datasheet of Zytel® 70G43HSLA BK099 from DuPont Engineering Polymers is provided by the international plastics database CAMPUS.

This datasheet includes:

  Zytel® 70G43HSLA BK099 | PA66-GF43 | DuPont Engineering Polymers
レオロジー特性乾燥/調湿単位テスト基準
成形収縮率, 平行 0.3 / * % ISO 294-4, 2577
成形収縮率, 直角 0.9 / * % ISO 294-4, 2577
機械的特性乾燥/調湿単位テスト基準
引張弾性率 14000 / 11000 MPa ISO 527-1/-2
破壊応力 220 / 160 MPa ISO 527-1/-2
破壊ひずみ 3 / 3.5 % ISO 527-1/-2
シャルピー衝撃強さ, +23°C 90 / 100 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 15 / - kJ/m² ISO 179/1eA
パンクチャー衝撃エネルギー, +23°C 4.4 / - J ISO 6603-2
熱的特性乾燥/調湿単位テスト基準
溶融温度, 10°C/min 262 / * °C ISO 11357-1/-3
ガラス転移点, 10°C/min 80 / * °C ISO 11357-1/-2
荷重たわみ温度, 1.80 MPa 235 / * °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 258 / * °C ISO 75-1/-2
酸素指数 24 / * % ISO 4589-1/-2
電気的特性.乾燥/調湿単位テスト基準
誘電正接, 100Hz 130 / - E-4 IEC 60250
誘電正接, 1MHz 150 / - E-4 IEC 60250
体積抵抗率 >1E13 / - Ohm*m IEC 60093
耐電圧 25 / - kV/mm IEC 60243-1
耐トラッキング性 600 / - - IEC 60112
その他の特性.乾燥/調湿単位テスト基準
吸水率 4.7 / * % Sim. to ISO 62
吸湿率 1.5 / * % Sim. to ISO 62
密度 1490 / - kg/m³ ISO 1183
材料特有の特性乾燥/調湿単位テスト基準
粘度数 120 / * cm³/g ISO 307, 1157, 1628
流動解析用データ単位テスト基準
溶融時の熱伝導率 0.25 W/(m K) -
機能
 引張弾性率-温度. , Zytel® 70G43HSLA BK099, PA66-GF43, DuPont
LTHA-破壊応力. 0mm, Zytel® 70G43HSLA BK099, PA66-GF43, DuPont
LTHA- 破壊ひずみ. 4mm, Zytel® 70G43HSLA BK099, PA66-GF43, DuPont
 LTHA-シャルピー衝撃強さ.(23゚C) 4mm, Zytel® 70G43HSLA BK099, PA66-GF43, DuPont
特殊な特性
成形加工法.
射出成形.
納入形状.
ペレット.
添加剤.
離型剤.
特殊な特性.
熱安定化.
領域別の利用可能性
耐薬品性
5wt%酢酸 (23゚C)
10wt%クエン酸 (23゚C)
10wt%乳酸 (23゚C)
36wt%塩酸 (23゚C)
40wt%硝酸 (23゚C)
38wt%硫酸 (23゚C)
5wt%硫酸 (23゚C)
40wt%硝酸 (23゚C)
塩基
35wt%水酸化ナトリウム (23゚C)
1wt%水酸化ナトリウム (23゚C)
10wt%水酸化アンモニウム (23゚C)
アルコール
イソプロピルアルコール23℃ (23゚C)
メタノール 23℃ (23゚C)
エタノール 23℃ (23゚C)
炭化水素
ヘキサン (23゚C)
トルエン (23゚C)
イソオクタン (23゚C)
ケトン系溶剤
アセトン (23゚C)
エーテル溶剤
ジエチルエーテル (23゚C)
鉱油
SAE 10W40 マルチグレードモーターオイル (23゚C)
SAE 10W40 マルチグレードモーターオイル (130゚C)
SAE 80/90 ハイポイドギアオイル (130゚C)
絶縁油 (23゚C)
標準燃料
ISO 1817液1 (60゚C)
ISO 1817液2 (60゚C)
ISO 1817液3 60℃ (60゚C)
ISO 1817液4 (60゚C)
標準燃料(ISO 1817液C)アルコールなし (23゚C)
標準燃料(ISO 1817液4)アルコールあり (23゚C)
ディーゼル燃料(ISO 1817液F) (23゚C)
ディーゼル燃料(ISO 1817液F) (90゚C)
ディーゼル燃料(ISO 1817液F) (>90゚C)
食塩水
10wt%塩化ナトリウム (23゚C)
10wt%次亜塩素酸ナトリウム (23゚C)
20wt%炭酸ナトリウム (23゚C)
2wt%炭酸ナトリウム (23゚C)
50wt%ジンクロメート (23゚C)
その他
エチルアセテート (23゚C)
過酸化水素 (23゚C)
DOT No.4ブレーキ液 (130゚C)
50wt%エチレングリコール水溶液 (108゚C)
1wt%ノニルフェノキシ-ポリエチレノキシ-エタノール水... (23゚C)
オレイン酸50%+オリーブオイル50% (23゚C)
水 (23゚C)
純水 (90゚C)
5wt%フェノール溶液 (23゚C)
Disclaimer
All data provided according to ISO 10350 for single points and ISO 11403 for multipoints.

Contact DuPont for Material Safety Data Sheet, general guides and/or additional information about ventilation, handling, purging, drying, etc.
Test temperatures are 23°C unless otherwise stated.

The DuPont Oval Logo, DuPont™, The miracles of science™ and ® are trademarks or registered trademarks of DuPont Company.
Copyright© 2013 E.I. du Pont de Nemours and Company. All Rights Reserved.

The information provided in this data sheet corresponds to our knowledge on the subject at the date of its publication.
This information may be subject to revision as new knowledge and experience becomes available.
The data provided fall within the normal range of product properties and relate only to the specific material designated; these data may not be
valid for such material used in combination with any other materials, additives or pigments or in any process, unless expressly indicated otherwise.
The data provided should not be used to establish specification limits or used alone as the basis of design; they are not intended to substitute
for any testing you may need to conduct to determine for yourself the suitability of a specific material for your particular purposes.
Since DuPont cannot anticipate all variations in actual end-use conditions DuPont makes no warranties and assumes no liability in connection
with any use of this information.
Nothing in this publication is to be considered as a license to operate under or a recommendation to infringe any patent rights.
DuPont advises you to seek independent counsel for a freedom to practice opinion on the intended application or end-use of our products.

CAUTION: DO NOT USE DUPONT MATERIALS IN MEDICAL APPLICATIONS INVOLVING IMPLANTATION IN THE HUMAN BODY OR
CONTACT WITH INTERNAL BODY FLUIDS OR TISSUES UNLESS THE MATERIAL HAS BEEN PROVIDED FROM DUPONT UNDER A
WRITTEN CONTRACT THAT IS CONSISTENT WITH DUPONT POLICY REGARDING MEDICAL APPLICATIONS AND EXPRESSLY
ACKNOWLEDGES THE CONTEMPLATED USE.

For further information, please contact your DuPont representative. You may also request a copy of DuPont POLICY Regarding Medical
Applications... H-50103-3 and DuPont CAUTION Regarding Medical Applications... H-50102-3.