Celanex 4305 is a 33% glass reinforced, toughened, thermoplastic
polyester.
polyester.
| 유변학적 특성 | 값 | 단위 | 시험규격 |
| 용융 부피 - 흐름 속도, MVR | 5.7 | cm³/10min | ISO 1133 |
| 온도 | 250 | °C | ISO 1133 |
| 하중 | 2.16 | kg | ISO 1133 |
| 기계적 특성 | 값 | 단위 | 시험규격 |
| 인장탄성률 | 9500 | MPa | ISO 527-1/-2 |
| 파단시 강도 | 110 | MPa | ISO 527-1/-2 |
| 파단시 신율 | 3 | % | ISO 527-1/-2 |
| 챠피 충격 강도 , +23°C | 54 | kJ/m² | ISO 179/1eU |
| 챠피 충격 강도, -30°C | 54 | kJ/m² | ISO 179/1eU |
| 챠피 노치드 충격 강도, +23°C | 13.1 | kJ/m² | ISO 179/1eA |
| 챠피 노치드 충격 강도, -30°C | 13.2 | kJ/m² | ISO 179/1eA |
| 열적 특성 | 값 | 단위 | 시험규격 |
| 녹는점, 10°C/min | 225 | °C | ISO 11357-1/-3 |
| 하중하에서의 변형온도, 1.80 MPa | 206 | °C | ISO 75-1/-2 |
| 하중하에서의 변형온도, 0.45 MPa | 224 | °C | ISO 75-1/-2 |
| 선형 열팽창 계수, 평행 | 20 | E-6/K | ISO 11359-1/-2 |
| 선형 열팽창 계수, 수직 | 65 | E-6/K | ISO 11359-1/-2 |
| 테스트 견본 생산 | 값 | 단위 | 시험규격 |
| ISO에 따른 공정 조건 | 7790 | - | ISO ....-2 |
| 사출성형: 용융수지온도 | 260 | °C | ISO 294 |
| 사출성형: 금형온도 | 82 | °C | ISO 10724 |
| 사출성형: 사출속도 | 300 | mm/s | ISO 294 |
| 사출성형: 유지압력 | 48 | MPa | ISO 294 |
특징
생산 공정
사출 성형
인도 유형
펠렛 (입자,알갱이)
부가물
윤활제
지역별 검색
Disclaimer
NOTICE TO USERS: Values shown are based on testing of laboratory test specimens and represent data that fall within the standard range of properties for natural material. These values alone do not represent a sufficient basis for any part design and are not intended for use in establishing maximum, minimum, or ranges of values for specification purposes. Colorants or other additives may cause significant variations in data values. Properties of molded parts can be influenced by a wide variety of factors including, but not limited to, material selection, additives, part design, processing conditions and environmental exposure. Any determination of the suitability of a particular material and part design for any use contemplated by the users and the manner of such use is the sole responsibility of the users, who must assure themselves that the material as subsequently processed meets the needs of their particular product or use. To the best of our knowledge, the information contained in this publication is accurate; however, we do not assume any liability whatsoever for the accuracy and completeness of such information. The information contained in this publication should not be construed as a promise or guarantee of specific properties of our products. It is the sole responsibility of the users to investigate whether any existing patents are infringed by the use of the materials mentioned in this publication. Moreover, there is a need to reduce human exposure to many materials to the lowest practical limits in view of possible adverse effects. To the extent that any hazards may have been mentioned in this publication, we neither suggest nor guarantee that such hazards are the only ones which exist. We recommend that persons intending to rely on any recommendation or to use any equipment, processing technique, or material mentioned in this publication should satisfy themselves that they can meet all applicable safety and health standards. We strongly recommend that users seek and adhere to the manufacturer's current instructions for handling each material they use, and to entrust the handling of such material to adequately trained personnel only. Please call the telephone numbers listed for additional technical information. Call Customer Services for the appropriate Materials Safety Data Sheets (MSDS) before attempting to process our products. The products mentioned herein are not intended for use in medical or dental implants.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012