CELSTRAN PA66-GF60-0104P10/11 | PA666-GF60 | Ticona
Informação do produto
60 % long glas fiber reinforced PA 66 with improved demolding
properties
Material code according to ISO 1043-1: PA66
Nylon 66/6 copolymer reinforced by 60 weight percent long glass
fibers with improved demolding propertiesThe pellets are cylindrical
and normally as well as the
embedded fibers 10 mm long.
Parts molded of CELSTRAN have outstanding mechanical properties such
as high strength and stiffness combined with high heat deflection.
The notched impact strength is increased at elevated and low
temperatures due to the fiber skeleton built in the parts. The long
fiber reinforcement reduces creep significantly.
The very isotropic shrinkage in the molded parts minimizes the
warpage.
Complex parts can be manufactured with high reproducibility by
injection molding.
Can be used for substituting die cast metal with the advantage of
Weight reduction, no corrosion problems, no post treatment
properties
Material code according to ISO 1043-1: PA66
Nylon 66/6 copolymer reinforced by 60 weight percent long glass
fibers with improved demolding propertiesThe pellets are cylindrical
and normally as well as the
embedded fibers 10 mm long.
Parts molded of CELSTRAN have outstanding mechanical properties such
as high strength and stiffness combined with high heat deflection.
The notched impact strength is increased at elevated and low
temperatures due to the fiber skeleton built in the parts. The long
fiber reinforcement reduces creep significantly.
The very isotropic shrinkage in the molded parts minimizes the
warpage.
Complex parts can be manufactured with high reproducibility by
injection molding.
Can be used for substituting die cast metal with the advantage of
Weight reduction, no corrosion problems, no post treatment
| Propriedades mecânicas | Seco / Cond | Unidade | Método de ensaio |
| Módulo de tração | 19500 / 14000 | MPa | ISO 527-1/-2 |
| Tensão na ruptura | 270 / 190 | MPa | ISO 527-1/-2 |
| Deformação na ruptura | 2 / 2 | % | ISO 527-1/-2 |
| Resistência ao impacto Charpy , +23°C | 95 / 95 | kJ/m² | ISO 179/1eU |
| Resistência ao impacto Charpy, -30°C | 85 / 90 | kJ/m² | ISO 179/1eU |
| Res. impacto Charpy c/entalhe, +23°C | 50 / 40 | kJ/m² | ISO 179/1eA |
| Res. impacto Charpy c/entalhe, -30°C | 45 / 45 | kJ/m² | ISO 179/1eA |
| Energia de perfuração, +23°C | 34 / - | J | ISO 6603-2 |
| Energia de perfuração, -30°C | 31 / - | J | ISO 6603-2 |
| Propriedades térmicas | Seco / Cond | Unidade | Método de ensaio |
| Temperatura de fusão, 10°C/min | 240 / * | °C | ISO 11357-1/-3 |
| Temperatura de deflexão térmica, 1.80 MPa | 240 / * | °C | ISO 75-1/-2 |
| Temperatura de deflexão térmica, 8.00 MPa | 220 / * | °C | ISO 75-1/-2 |
| Outras propriedades | Seco / Cond | Unidade | Método de ensaio |
| Densidade | 1670 / 1670 | kg/m³ | ISO 1183 |
| Propriedades específicas do material | Seco / Cond | Unidade | Método de ensaio |
| Índice de viscosidade | 120 / * | cm³/g | ISO 307, 1157, 1628 |
Disclaimer
NOTICE TO USERS: Values shown are based on testing of laboratory test specimens and represent data that fall within the standard range of properties for natural material. These values alone do not represent a sufficient basis for any part design and are not intended for use in establishing maximum, minimum, or ranges of values for specification purposes. Colorants or other additives may cause significant variations in data values. Properties of molded parts can be influenced by a wide variety of factors including, but not limited to, material selection, additives, part design, processing conditions and environmental exposure. Any determination of the suitability of a particular material and part design for any use contemplated by the users and the manner of such use is the sole responsibility of the users, who must assure themselves that the material as subsequently processed meets the needs of their particular product or use. To the best of our knowledge, the information contained in this publication is accurate; however, we do not assume any liability whatsoever for the accuracy and completeness of such information. The information contained in this publication should not be construed as a promise or guarantee of specific properties of our products. It is the sole responsibility of the users to investigate whether any existing patents are infringed by the use of the materials mentioned in this publication. Moreover, there is a need to reduce human exposure to many materials to the lowest practical limits in view of possible adverse effects. To the extent that any hazards may have been mentioned in this publication, we neither suggest nor guarantee that such hazards are the only ones which exist. We recommend that persons intending to rely on any recommendation or to use any equipment, processing technique, or material mentioned in this publication should satisfy themselves that they can meet all applicable safety and health standards. We strongly recommend that users seek and adhere to the manufacturer's current instructions for handling each material they use, and to entrust the handling of such material to adequately trained personnel only. Please call the telephone numbers listed for additional technical information. Call Customer Services for the appropriate Materials Safety Data Sheets (MSDS) before attempting to process our products. The products mentioned herein are not intended for use in medical or dental implants.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.