- Formerly Makrolon KU1-1248
- MVR (300 °C/1.2 kg) 7.0 cm3/10 min
- food contact quality
- medium viscosity
- impact modified
- available in light colors only
| Propriedades reológicas | Valor | Unidade | Método de ensaio |
| Índice de fluidez volumétrico, MVR | 7 | cm³/10min | ISO 1133 |
| Temperatura | 300 | °C | ISO 1133 |
| Carga | 1.2 | kg | ISO 1133 |
| Contração após a moldagem, paralelo | 0.8 | % | ISO 294-4, 2577 |
| Contração após a moldagem, perpendicular | 0.8 | % | ISO 294-4, 2577 |
| Propriedades mecânicas | Valor | Unidade | Método de ensaio |
| Módulo de tração | 2250 | MPa | ISO 527-1/-2 |
| Tensão no escoamento | 61 | MPa | ISO 527-1/-2 |
| Deformação no escoamento | 6 | % | ISO 527-1/-2 |
| Deformação nominal na ruptura | >50 | % | ISO 527-1/-2 |
| Resistência ao impacto Charpy , +23°C | N | kJ/m² | ISO 179/1eU |
| Resistência ao impacto Charpy, -30°C | N | kJ/m² | ISO 179/1eU |
| Perfuração - força máxima, +23°C | 5200 | N | ISO 6603-2 |
| Perfuração - força máxima, -30°C | 6100 | N | ISO 6603-2 |
| Energia de perfuração, +23°C | 55 | J | ISO 6603-2 |
| Energia de perfuração, -30°C | 60 | J | ISO 6603-2 |
| Propriedades térmicas | Valor | Unidade | Método de ensaio |
| Temp. de transição vítrea, 10°C/min | 148 | °C | ISO 11357-1/-2 |
| Temperatura de deflexão térmica, 1.80 MPa | 125 | °C | ISO 75-1/-2 |
| Temperatura de deflexão térmica, 0.45 MPa | 139 | °C | ISO 75-1/-2 |
| Temperatura de amolecimento Vicat, 50°C/h 50N | 146 | °C | ISO 306 |
| Coef. de expansão térmica linear, paralelo | 70 | E-6/K | ISO 11359-1/-2 |
| Coef. de expansão térmica linear, perpend. | 70 | E-6/K | ISO 11359-1/-2 |
| Flamabilidade a 1.5mm esp. nom. | HB | class | IEC 60695-11-10 |
| Espessuras do tubo de teste | 1.5 | mm | IEC 60695-11-10 |
| Flamabilidade conforme índice de oxigênio | 30 | % | ISO 4589-1/-2 |
| Propriedades elétricas | Valor | Unidade | Método de ensaio |
| Constante dielétrica, 100Hz | 3.1 | - | IEC 60250 |
| Constante dielétrica, 1MHz | 3 | - | IEC 60250 |
| Fator de dissipação dielétrica, 100Hz | 12 | E-4 | IEC 60250 |
| Fator de dissipação dielétrica, 1MHz | 120 | E-4 | IEC 60250 |
| Resistividade volumétrica específica | >1E13 | Ohm*m | IEC 60093 |
| Resistividade superficial específica | >1E15 | Ohm | IEC 60093 |
| Resistência elétrica | 34 | kV/mm | IEC 60243-1 |
| Índice comparativo de linha de fuga | 225 | - | IEC 60112 |
| Outras propriedades | Valor | Unidade | Método de ensaio |
| Absorção de água | 0.4 | % | Sim. to ISO 62 |
| Absorção de umidade | 0.12 | % | Sim. to ISO 62 |
| Densidade | 1200 | kg/m³ | ISO 1183 |
| Propriedades específicas do material | Valor | Unidade | Método de ensaio |
| Transmitância luminosa | 89 | % | ISO 13468-1, -2 |
| Propriedades para cálculos reológicos | Valor | Unidade | Método de ensaio |
| Densidade do fundido | 1020 | kg/m³ | - |
| Condutividade térmica do fundido | 0.214 | W/(m K) | - |
| Capacidade térmica específica do fundido | 2100 | J/(kg K) | - |
| Difusividade térmica | 1E-7 | m²/s | - |
| Temperatura de ejeção | 130 | °C | - |
| Produção de amostra para teste | Valor | Unidade | Método de ensaio |
| Moldagem por injeção, temperatura da massa | 300 | °C | ISO 294 |
| Moldagem por injeção, temperatura do molde | 80 | °C | ISO 10724 |
| Moldagem por injeção, velocidade de injeção | 200 | mm/s | ISO 294 |
Bayer MaterialScience AG
The manner in which you use and the purpose to which you put and utilize our products, technical assistance and information (whether verbal, written or by way of production evaluations), including any suggested formulations and recommendations, are beyond our control. Therefore, it is imperative that you test our products, technical assistance and information to determine to your own satisfaction whether they are suitable for your intended uses and applications. This application-specific analysis must at least include testing to determine suitability from a technical as well as health, safety and environmental standpoint. Such testing has not necessarily been done by us. Unless we otherwise agree in writing, all products are sold strictly pursuant to the terms of our standard conditions of sale which are available upon request. All information and technical assistance is given without warranty or guarantee, and is subject to change without notice. It is expressly understood and agreed that you assume and hereby expressly release us from all liability, in tort, contract or otherwise, incurred in connection with the use of our products, technical assistance and information. Any statement or recommendation not contained herein is unauthorized and shall not bind us. Nothing herein shall be construed as a recommendation to use any product in conflict with patents covering any material or its use. No license is implied or in fact granted under the claims of any patent. Unless specified to the contrary, the property values given have been established on standardized test specimens at room temperature. The figures should be regarded as typical values only and not as binding limiting values. Please note that the properties can be affected by the design of the mold/die, the processing conditions and coloring. With respect to health, safety and environment precautions, the relevant Material Safety Data Sheets (MSDS) and product labels must be observed prior to working with our products.
BMS Medical Grades
BMS Products that are designated as "Medical Grade", e.g., plastics, sheets, and films, meet certain biocompatibility test requirements of ISO Standard 10993-1: "Biological Evaluation of Medical Devices" for the categories including: 1) skin contact, 2) up to 24 hours contact with circulating blood, tissue, bone, and dentin, 3) up to 30 days contact with mucosal membranes, compromised surfaces, and blood path, indirect. BMS Products designated as "Medical Grade" shall not be considered candidates for the following types of Medical Applications unless BMS explicitly agrees, in writing, to sell such products for such applications: a) cosmetic, reconstructive, or reproductive implant applications; b) any other bodily implant applications; c)applications involving contact with or storage of human tissue, blood, or other bodily fluids, for greater than 30 days; or d) applications having greater than 24 hours contact with circulating blood, tissue, bone and dentin. The biocompatibility testing referenced above cannot assure the biocompatibility of final or intermediate products made from BMS Products or the suitability of such products for their use in a Medical Application, i.e., the test data cannot be used to conclude that any medical devices manufactured from the BMS Products meet the necessary requirements of ISO Standard 10993-1. It is the sole responsibility of the manufacturer of final end-use product to conduct all necessary tests (including biocompatibility tests) and inspections and to evaluate the final product under actual end-use requirements. The designation as "Medical Grade" does not mean that BMS or anyone else has determined that the product is suitable for use in any particular Medical Application. BMS makes no representations regarding the suitability of a BMS Product for a particular Medical Application or final enduse product. A determination that the BMS Product is suitable for use in a particular Medical Application or final end-use product can only be made by the purchaser of the BMS product who utilizes it in a Medical Application and conducts all necessary testing and evaluation to support such a determination.
Appropriate Use of BMS Products in a Medical Application
BMS has not performed clinical medical studies concerning the use of BMS Products. Moreover, BMS has neither sought nor received approval from the United States Food and Drug Administration (FDA) or other competent authorities from other regions for the use of BMS Products in a Medical Application. BMS makes no representations or warranty regarding (and accepts no responsibility for determining) either: (a) the suitability of a BMS Product for a particular Medical Application or final end-use product or (b) the adequacy of any warning relating to a BMS Product or particular Medical Application or final end-use product. The suitability of BMS Products in a given end-use environment is dependent upon various conditions including, without limitation, chemical compatibility, method of manufacture, temperature, part design, sterilization method, residual stresses, and external loads. It is the sole responsibility of the manufacturer of the final end-use product to determine the suitability (including biocompatibility) of all raw materials and components, including any BMS Products, in order to ensure that the final product: - meets relevant biocompatibility requirements and is otherwise safe for its end-use, - performs or functions as intended, - is suitable for its intended use, and - complies with all applicable FDA and other regulatory requirements. It also is the sole responsibility of the manufacturer of the final end-use product to conduct all necessary tests and inspections and to evaluate the final product under actual end-use requirements and to adequately advise and warn purchasers, users, and/or learned intermediaries (such as physicians) of pertinent risks and fulfill any postmarket surveillance obligations. Any decision regarding the appropriateness of a particular medical product in a particular clinical or Medical Application should be based on the judgment of the manufacturer, seller, the competent authority, and the treating physician. BMS cannot weigh the benefits against the risks of a medical device and cannot offer a medical or legal judgment on the safety or efficacy of the use of a BMS Product in a specific Medical Application. Terms in capital letters as used herein shall have the same meaning as defined in the "GUIDANCE ON USE OF BAYER MATERIALSCIENCE PRODUCTS IN A MEDICAL APPLICATION" which can be found under (see here). It is the customer's responsibility to thoroughly review the Guidance Document in detail and to diligently consider its content prior to any use of BMS Products in Medical Applications. For further information on our Medical Grades please see our brochure "Makrolon, Apec and Bayblend for medical devices".
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012