材料文字说明
Product-nomenclature according to ISO 1874:
PA612, MHR, 18-090, GF30
Product Attributes
| Hydrolysis resistant, Improved alcohol resistance, Improved heat resistance, Improved UV resistance (outdoor use) |
Markets
| Automotive | |
| Air intake sytems, Compressed air systems, Hydraulic systems, Automotive electr. and electronics, lighting, Cooling and climate control, Fuel systems, Powertrain and Chassis , Interior, Exterior | |
| Electricals & Electronics | |
| Electrical appliances, Electrical equipment, Connectors, Mobile phones and other portable devices, Lighting | |
| Industry & Consumer goods | |
| Heating systems, Housewares, Hydraulics & Pneumatics, Mechanical Engineering, Power transmission, Sports & Leisure, Tools & Accessories |
| 机械性能 | 干 / 已调节 | 单位 | 测试标准 |
| 拉伸模量 | 9500 / 7500 | MPa | ISO 527-1/-2 |
| 断裂应力 | 150 / 115 | MPa | ISO 527-1/-2 |
| 断裂伸长率 | 4.5 / 6.5 | % | ISO 527-1/-2 |
| 无缺口简支梁冲击强度, +23°C | 90 / 90 | kJ/m² | ISO 179/1eU |
| 无缺口简支梁冲击强度, -30°C | 95 / 90 | kJ/m² | ISO 179/1eU |
| 简支梁缺口冲击强度, +23°C | 15 / 16 | kJ/m² | ISO 179/1eA |
| 简支梁缺口冲击强度, -30°C | 10 / 10 | kJ/m² | ISO 179/1eA |
| 热性能 | 干 / 已调节 | 单位 | 测试标准 |
| 熔融温度, 10°C/min | 215 / * | °C | ISO 11357-1/-3 |
| 热变形温度, 1.80 MPa | 185 / * | °C | ISO 75-1/-2 |
| 热变形温度, 8.00 MPa | 110 / * | °C | ISO 75-1/-2 |
| 线性热膨胀系数, 平行 | 30 / * | E-6/K | ISO 11359-1/-2 |
| 线性热膨胀系数, 垂直 | 100 / * | E-6/K | ISO 11359-1/-2 |
| 厚度为h时的燃烧性 | HB / * | class | IEC 60695-11-10 |
| 测试用试样的厚度 | 0.8 / * | mm | IEC 60695-11-10 |
权利义务的法律声明
EMS-CHEMIE AG Business Unit EMS-GRIVORY Homepage : EMS-GRIVORY eMail : welcome@emsgrivory.com The values are intended to serve as an aid in preselecting materials and for an overview of the EMS-GRIVORY product range. The information contained in this publication is based on our present knowledge and experience. The given figures and data are guidance values and do not represent binding material specifications. No warranties of any kind, either express or implied, including warranties of merchantability or fitness for a particular purpose, are given regarding products, design, data and information. The customer is not released from his obligation to investigate the products fitness and the suitability for the intended application, compliance with legal requirements and intellectual property rights. We reserve the right to change the information at any time and without prior notice. The information in this publication is not to be considered a contractual obligation and any liability whatsoever is expressly declined. For further questions about our products please contact our experts.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012