PBT, 12 % glass fibres, injection moulding, flame retardant
流变性能价值单位测试标准
熔体体积流动速度, MVR 37 cm³/10min ISO 1133
温度 260 °C ISO 1133
载荷 2.16 kg ISO 1133
模塑收缩率, 平行 0.8 % ISO 294-4, 2577
模塑收缩率, 垂直 1.1 % ISO 294-4, 2577
机械性能价值单位测试标准
拉伸模量 5700 MPa ISO 527-1/-2
断裂应力 100 MPa ISO 527-1/-2
断裂伸长率 2.5 % ISO 527-1/-2
拉伸蠕变模量, 1h 5500 MPa ISO 899-1
拉伸蠕变模量, 1000h 5000 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C 30 kJ/m² ISO 179/1eU
无缺口简支梁冲击强度, -30°C 30 kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 10 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 10 kJ/m² ISO 179/1eA
热性能价值单位测试标准
熔融温度, 10°C/min 225 °C ISO 11357-1/-3
热变形温度, 1.80 MPa 185 °C ISO 75-1/-2
热变形温度, 0.45 MPa 205 °C ISO 75-1/-2
维卡软化温度, 50°C/h 50N 205 °C ISO 306
线性热膨胀系数, 平行 40 E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 100 E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 V-0 class IEC 60695-11-10
测试用试样的厚度 1.5 mm IEC 60695-11-10
厚度为h时的燃烧性 V-0 class IEC 60695-11-10
测试用试样的厚度 0.8 mm IEC 60695-11-10
燃烧性-氧指数 32 % ISO 4589-1/-2
电性能价值单位测试标准
相对介电常数., 100Hz 3.6 - IEC 60250
相对介电常数., 1MHz 3.4 - IEC 60250
介质损耗因子, 100Hz 40 E-4 IEC 60250
介质损耗因子, 1MHz 190 E-4 IEC 60250
体积电阻率 1E11 Ohm*m IEC 60093
表面电阻率 >1E15 Ohm IEC 60093
介电强度 29 kV/mm IEC 60243-1
相对漏电起痕指数 200 - IEC 60112
其它性能价值单位测试标准
吸水性 0.3 % 类似ISO 62
吸湿性 0.1 % 类似ISO 62
密度 1530 kg/m³ ISO 1183
试样制备条件价值单位测试标准
注塑, 熔体温度 260 °C ISO 294
注塑, 模具温度 80 °C ISO 10724
典型数据
加工方法
注塑
供货形式
粒料
地区供应
权利义务的法律声明
This information and our  technical advice - whether verbal, in  writing
or by way of trials - are  given in good faith but without warranty, and
this  also  applies  where  proprietary  rights  of  third  parties  are
involved.  Our advice does not release you from  the obligation to check
its validity and to test our  products  as to their  suitability for the
intended processes and uses.  The  application, use  and  processing  of
our products and the products manufactured  by  you  on the basis of our
technical  advice  are  beyond our control and, therefore, entirely your
own  responsibility.  Our  products  are  sold  in  accordance  with our
General  Conditions of Sale and Delivery.
The values  stored in the databank should only be used as guidelines for
component   design.  In  giving  these  values  neither  guarantee,  nor
assurance of particular material properties can be given.

techcenter.lanxess.com

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012